A road subgrade can appear firm before winter and lose support when spring thaw brings water back into its pores. For a contractor, that change matters more than how a soil performs on a dry day. Polypropylene (PP) fibers can help a compacted soil retain strength through freezing and thawing, but the correct fiber length and dosage depend on the soil, water, compaction, and the strength target.
At Shandong Jianbang Chemical Fiber Co., Ltd., we supply Ecocretefiber™ fibers for cementitious and other engineered materials. When a project team considers PP fiber for soil, we start with the site soil and a controlled trial. A published laboratory comparison of fiber modified soft soil gives a useful example. It also shows why a promising 0.3% result should guide testing rather than become a universal recipe.

Why Freeze Thaw Weakens A Road Subgrade
Frost action needs a frost susceptible soil, freezing conditions, and water. The Federal Highway Administration’s geotechnical guidance identifies spring thaw weakening and winter heave as separate problems. Water can move toward a freezing zone and form ice lenses. When that ice melts, the soil can be wet and less able to support loads.
A fiber changes how part of the soil skeleton resists deformation. Randomly distributed filaments can cross local zones where particles tend to separate. Soil particles grip the fiber surface, and the fiber can carry tension when the soil itself has limited tensile resistance. This is a practical explanation of reinforcement, but its scale depends on the fiber interface, orientation, mixing, and confinement.
Strength retention is not the same as frost heave control. A compression test after thaw can show that a reinforced specimen still carries a load. It does not by itself measure vertical heave, water migration, permeability, or the pavement’s long term movement. A cold region pavement still needs suitable drainage, grading, frost depth design, and an appropriate structural section. FHWA guidance describes those broader subgrade measures, including the effect of water availability on heave. See the FHWA discussion of frost and water.
What The Soil And Fiber Experiment Actually Tested
A 2020 study by Li Junfa in the Journal of Wuhan University of Technology (Transportation Science and Engineering) used a soft soil collected at a depth of 3.5 m in the eastern Songliao Plain. Its reported liquid limit was 42.8%, plastic limit 28.2%, maximum dry density 1.768 g/cm³, and optimum water content 18.6%. The test team compacted cylindrical samples to a target of 98% and used six specimens in each test group.
The researchers compared nominal fiber lengths of 6, 9, and 12 mm and contents of 0.1%, 0.2%, 0.3%, 0.4%, and 0.5%. Those percentages are fiber mass divided by dry soil mass. For example, 0.3% means 3 kg of fiber per 1,000 kg of dry soil. It is not 0.3% of wet soil and it is not a concrete dosage in kg/m³.
Each freeze thaw cycle held the specimen at -15°C for 12 hours and then at 20°C for 12 hours. The groups received 0, 5, 10, 15, or 20 cycles. The researchers measured shear behavior with unconsolidated undrained triaxial compression under confining pressures of 50, 100, and 200 kPa. They also ran unconfined compression tests. The specimen diameter was 39.1 mm and its height was 80 mm.
| Trial variable | Values used in the experiment | Why it matters |
| PP fiber content | 0.1% to 0.5% of dry soil mass | Changes the amount of reinforcement and the risk of poor dispersion |
| Fiber cut length | 6, 9, and 12 mm | Changes possible anchorage and the ease of uniform mixing |
| Freeze thaw exposure | 0, 5, 10, 15, and 20 cycles | Shows how the tested strength changed under this one thermal schedule |
| Strength measurement | UU triaxial shear and unconfined compression | Answers two related but different strength questions |
The specimens and fiber grades used in that experiment define its results. The study did not establish a universal specification for all soil types or every available PP fiber. Its fiber specification should also not be substituted for an Ecocretefiber™ product data sheet.

What Happened As The Samples Froze And Thawed
At a given fiber content and cut length, the reported shear and compressive strengths generally fell as the cycles increased. The largest changes occurred earlier in the sequence. The researchers observed a flatter response after about 15 cycles in their setup.
The detailed results and conclusion report that the average shear strength of the fiber modified soil was 10.7% lower after 15 cycles than before cycling. At 20 cycles, the average reduction was 12.1%. For unconfined compressive strength, the detailed results give average reductions of 34.5% after 15 cycles and 38.0% after 20 cycles. Compression therefore showed a much larger percentage loss than shear in this experiment.
These percentages describe change from the corresponding fiber modified specimens at zero cycles. They do not quantify the benefit over an unreinforced control soil. That distinction matters when a bid or design report asks, “How much better is this product than the untreated soil?” A side by side untreated control is needed to answer that question for the project soil.
The paper’s abstract and detailed body differ on the 15 cycle compressive strength percentage. We use the detailed results and conclusion, which both state 34.5%, and advise checking the original experimental record before quoting that figure in a formal specification. The difference does not change the main trend: freeze thaw still weakened the tested fiber modified soil.
A stable trend after 15 laboratory cycles is not proof that 15 cycles represent every climate or design life. Field temperatures, moisture supply, freezing rate, and traffic differ from this controlled exposure. The appropriate laboratory conditioning and acceptance threshold belong in the project’s geotechnical test plan.

Why The Best Tested Dosage Was 0.3 Percent
For a fixed length and comparable test conditions, strength first rose and then fell as the researchers added more fiber. Both the shear and unconfined compression results peaked at 0.3% of dry soil mass among the five contents tested. More fiber was not automatically better.
When content increased from 0.1% to 0.3%, the reported average shear strength gains depended on fiber length and confining pressure. They were at least 3.2% across the comparisons described by the researchers. The average unconfined compression gains were 136% for the 6 mm series, 82% for the 9 mm series, and 79% for the 12 mm series. Each gain compares two fiber reinforced mixtures in the experiment. It should not be described as a gain over untreated soil.
At the same cycle count and length, the 0.3% mixture also averaged 9.8% higher compressive strength than the 0.4% mixture in the reported comparison. A likely engineering interpretation is that added filaments eventually become harder to spread evenly and compact. The study did not isolate a microscopic mechanism, so we would confirm that interpretation by examining clumps, voids, water content, and density in a new trial.
Use 0.3% as a trial center when the project soil and fiber resemble the tested system. Test a lower and a higher level beside it. If a different soil needs a different amount, follow the measured result. Record the percentage on a dry mass basis on every trial sheet so a plant operator does not mistake it for kg/m³ of concrete.
Fiber Length Changes Shear And Compression Differently
In this comparison, unconfined compressive strength generally rose as cut length increased from 6 to 9 to 12 mm. The improvement from 9 to 12 mm was relatively small. Across the five dosage series, the average reported gains for that last step were 7.6%, 2.9%, 4.3%, 4.3%, and 5.4%.
The shear result had a different pattern. At lower fiber content, shear strength reached a high point at 9 mm and then declined at 12 mm. At contents of 0.3% or higher, the reported shear strength generally continued to rise with length. The original researchers recommended 9 mm as a balanced length for their soil and testing conditions.
A longer fiber can bridge more space, yet it may also resist uniform mixing or change how the material compacts. A short fiber may disperse easily but provide less effective anchorage. For a site project, choose the length by the governing strength requirement and by what the crew can distribute throughout the full compacted layer.
Ecocretefiber™ currently lists monofilament PP fiber in several cut lengths, including 6, 9, and 12 mm. Its published product page describes a density of 0.91 g/cm³ and a range of diameters. The experimental paper listed a different fiber density and other grade properties. Matching the cut length does not mean the two fibers are identical or will produce the same soil strength. Ask our team for the current grade data sheet and qualify the chosen material in your own soil.

How To Turn The Findings Into A Useful Trial
Start with a representative sample from the construction area. Determine its grading, plasticity, natural water content, compaction curve, and relevant frost susceptibility. A soft soil from one region may behave differently from a silty embankment, a granular fill, or a lime treated soil. If the project uses a binder, treat that as a new mixture and test it as such.
Prepare a clear control set. Include the untreated soil at the same target moisture and compaction, then compare fiber lengths and dry mass contents under the same conditioning. Record dry soil mass, fiber mass, water addition, actual moisture, and achieved dry density for each batch. Set a mixing order that lets fibers separate without making balls. The exact sequence should be validated on the planned equipment.
Compact the test specimens with a controlled method and measure their actual density. Matching nominal fiber dose without matching density can produce a misleading strength comparison. Condition parallel specimens through the project’s selected freeze thaw schedule and protect them from uncontrolled water loss or gain. Test uncycled and cycled sets, and document any cracking or shape change.
Choose the performance measure before seeing the results. ASTM D2166/D2166M-24 covers unconfined compressive strength of suitable cohesive soils. ASTM D2850-26 covers unconsolidated undrained triaxial compression with confinement. The methods address different stress conditions and their numerical results should not be exchanged. Follow the contract’s current edition and the laboratory’s approved procedure.
For pavement design, consider whether the project also needs direct evidence on heave and thaw weakening. The discontinued ASTM D5918-13e1 historically addressed those outcomes, but it was withdrawn in 2022. Do not present it as a current active acceptance standard. Agree on an appropriate current test program with the geotechnical designer and owner. A post thaw strength result alone cannot establish heave control.

Mixing And Site Checks Before Full Scale Placement
A fiber can help only when it reaches the soil uniformly. Check whether the selected fiber opens easily in the actual mixer. Inspect several samples across a batch, including material from the beginning and end of discharge. Look for bundles and areas with unusually high fiber content. Then confirm that the mix can still be spread and compacted at the intended lift thickness.
Keep the dry mass basis visible in the field calculation. If a batch contains 2,000 kg of dry soil, 0.3% corresponds to 6 kg of fiber. The wet soil mass may be higher and changes as water content changes. A site crew should therefore convert the target from measured dry mass or an agreed dry density and batch volume, rather than guess from a nominal truckload weight.
At the trial pad, measure moisture and in place density and check the finished surface. Take specimens or cores under an agreed sampling plan. A good laboratory result will not rescue a layer with poor compaction, wet pockets, or uneven distribution. Drainage and pavement design remain part of the frost solution, as FHWA’s subgrade treatment guidance makes clear.
Shandong Jianbang can provide fiber samples and current specifications for a qualification trial. Tell us the soil classification, target fiber length, planned mixing equipment, moisture range, and required tests. We can help select a PP grade to test, while the project engineer sets the acceptance criteria.

Questions Buyers And Engineers Often Ask
Does 0.3 Percent Mean 0.3 Kilograms Per Cubic Meter
No. In this study, it means 0.3 kg fiber per 100 kg dry soil, or 3 kg per 1,000 kg dry soil. A dosage in kg/m³ depends on the compacted dry density. Concrete fiber dosing conventions should not be copied into a soil trial.
Did The Fiber Prevent Frost Heave
The experiment reported post cycle shear and compression tests. It did not provide a direct frost heave measurement or an untreated control for a quantified treatment benefit. Those outcomes need separate evaluation for the project.
Should Every Cold Region Project Use 15 Freeze Thaw Cycles
No. The reported strength changes became smaller after about 15 cycles under one laboratory schedule. A project should select exposure and acceptance rules that reflect its climate, water conditions, materials, and contract requirements.
Is 12 Millimeters Better Than 9 Millimeters
It depends on the target. The study found a small average compression gain from 9 to 12 mm, while its shear trends depended on content and confinement. A 9 mm fiber was the researchers’ balanced recommendation for their test soil. Confirm the choice in a project trial.
Can A Concrete PP Fiber Be Put Straight Into Soil
A product sold for concrete may be available in a suitable cut length, but its surface, diameter, dispersion, and performance in soil need qualification. Use the product data sheet and a soil specific mixing and strength test before specifying it.
Conclusion
The most useful lesson is the shape of the response. In the tested soft soil, repeated freezing and thawing reduced strength, a middle fiber content performed best among five trial levels, and the best cut length depended on whether shear or compression was the main concern. The 0.3% dry soil dosage and 9 mm recommendation are sound starting points for a comparable trial, not guaranteed design values for another soil or an Ecocretefiber™ grade.
Shandong Jianbang Chemical Fiber Co., Ltd. supplies Ecocretefiber™ PP fiber options and can help a project team choose samples for laboratory and field evaluation. Contact our team with your soil data, conditioning plan, and acceptance targets. A reproducible trial gives a much stronger basis for a purchase and a subgrade specification.